Shutdown corrosion: why chloride salts in ash rust grate bars at room temperature
Grate bars are usually treated as high-temperature parts, and every discussion circles around melting, oxide spalling and thermal cracking above 800℃. Workshop inspection often shows something else: spares that were fine at the last maintenance season sit in the warehouse or inside the furnace for a summer, and at installation the pin holes are rusted solid, the working face has a film of rust, and there are pits eaten into the surface. Shutdown is not a corrosion-free period; it is a different mechanism — room-temperature electrochemical corrosion instead of high-temperature oxidation, with the electrolyte supplied by the ash.

1. Corrosion during shutdown is not slow, it just does not smoke
The corrosion rate of carbon steel in air is not linear in relative humidity: above a critical value of about 60% it rises steeply, and the 60%–100% range runs 100–1000 times the rate of the 30%–55% range (the relationship curve cited in Annex B of DL/T 956-2017). That curve is what dry lay-up of idle boilers is built on: hold the internal relative humidity below the critical value and corrosion is suppressed.
The grate side works the same way, except that what stays on the grate is not water but ash. Salts in the ash pull the critical humidity down to a level a maintenance site cannot reach.
2. Ash is a salt store: deliquescence humidity decides when it turns wet
Chloride salts take up moisture from the air until a saturated solution forms on their own surface; that transition point is the deliquescence relative humidity (DRH). DRH of common salts at 25℃: calcium chloride hexahydrate 28.1%, magnesium chloride hexahydrate 32.8%, potassium carbonate 43.2% (essentially unchanged between 15–25℃), sodium chloride 75%; potassium chloride is higher but falls with temperature — 88.6% at 0℃ and 78.5% at 90℃.
The consequence: if the ash contains a salt such as calcium chloride, it is already wet at 28% relative humidity. A rainy season in the south, or a maintenance period with a wide day-night temperature swing in the north, takes both the furnace and the warehouse past that value easily. Once a liquid film forms, chloride ions pit the metal, the rust layer is porous and protects nothing, and the attack goes deeper. Moisture uptake by chlorides in biomass and waste ash is identified in the published literature as a main cause of low-temperature corrosion (npj Materials Degradation review, 2025).
The calcium chloride in the ash is not a contaminant: it forms from calcium in the fuel reacting with hydrogen chloride in the flue gas, which is why a high-chlorine fuel leaves ash that picks up moisture more readily than coal ash does during shutdown.
3. Start-up and shutdown: water condenses first, then that water becomes the electrolyte
The water dew point depends on the water vapour content of the flue gas. Calculated at atmospheric pressure: 10% vol water vapour gives a dew point near 46℃, 15% near 54℃, 20% near 60℃. Biomass fuel carries more moisture, the flue gas holds more water vapour, and the dew point sits higher than with coal.
The same review notes that water dew-point corrosion is most often encountered at partial load and during start-up and shutdown periods — the times when metal temperature drops below the dew point. On a cold start the grate and the furnace walls have not heated up, flue gas temperature is low and moisture content high, so condensation is almost certain; that water lands on an ash-covered surface and immediately becomes a chloride-bearing acidic film. Shutdown runs the same way: the furnace is still cooling, moist air gets in, and the ash is still lying on the grate.
4. Shutdown procedure: getting the sequence right beats buying more spares
- Remove the ash first, then talk about drying. Leave the ash and every later dehumidification step is just a water supply for the salts. Soot blowing is safer than water washing; if the furnace has been washed, it must be dried through and through, otherwise the wash was an addition of water
- Close up and dehumidify. The dry-air method in DL/T 956-2017 keeps relative humidity at each exhaust point within 30%–50%, and the desiccant method requires internal relative humidity no higher than 60%; the desiccant quantity that guideline gives as a reference is 2 kg/m³ of colour-indicating silica gel. An industrial furnace is hard to seal, so getting below 50% is not easy, but pushing humidity below 60% and closing manholes and air dampers tightly costs very little
- Prevent condensation before controlling humidity. Another rule in that guideline is to keep the exhaust-side air temperature 5℃ above the surrounding ambient. For a furnace that means do not leave the furnace doors open for ventilation on cold days — ventilation removes moisture, but it also drags metal temperature below the dew point
- Treat bolts and pin holes separately. What rusts solid during shutdown is not the working face but the mating faces: coating pin holes and bolts with high-temperature anti-seize before assembly is far less work than cutting them out afterwards
5. Spare storage and purchase clauses: the part worth writing into the technical agreement
Spare grate bars are castings with mostly uncoated working faces, so storage conditions decide what arrives on site:
- Keep the original packaging. GB/T 4879-2016 (rustproof packaging) sets grade 1 (2-year protection), grade 2 (1 year) and grade 3 (0.5 year); order long-stored spares at grade 1, and open or half-open yard storage means giving up the packaging altogether
- Off the ground, on timber, out of rain, out of condensation. A casting stood straight on the floor draws moisture up from the ground, and in a warehouse with a wide day-night swing a metal surface colder than the dew point condenses water
- Judge rusted parts before deciding: light surface rust can be cleaned to Sa2½ of GB/T 8923.1 and used; if there are pits, or mating-face rust that affects the assembly clearance, do not grind it to fit — grinding changes dimensions, while assembly clearance is a design value
- When ordering, write the rustproof packaging grade, the transport method and the storage period into the technical agreement; it is worth more than an argument afterwards. For how to fix the specification and quantity, see the spare parts list
Shutdown corrosion rarely perforates a grate bar in one go. The cost shows up elsewhere: mating faces rusted solid stretch the maintenance schedule, pits become the starting point of the next thermal crack (see the four failure modes), and there is the quality argument about a new spare that arrives already rusty.

References
- Jafarihonar F., Vainio E., Hupa L., Hupa M., Low-temperature corrosion in large-scale biomass boilers, npj Materials Degradation, 2025, 9
- Peng C., Chen L., Tang M., A database for deliquescence and efflorescence relative humidities of compounds with atmospheric relevance, Fundamental Research, 2022, 2(4): 578–587
- Eggert G., Saturated salt solutions in showcases: humidity control and pollutant absorption, Heritage Science, 2022, 10
- Vainio E., DeMartini N., Hupa L., Åmand L., Hygroscopic Properties of Calcium Chloride and Its Role on Cold-End Corrosion in Biomass Combustion, Energy & Fuels, 2019, 33: 11913–11922
- DL/T 956-2017, Guideline for lay-up of thermal power equipment in fossil plants
- GB/T 4879-2016, Rustproof packaging
- GB/T 8923.1-2011, Preparation of steel substrates before application of paints, part 1